Material Amount Batch Subtotal
Nepheline Syenite (Theoretical) 30
Silica 30
Gerstley Borate 20
Whiting 10
EPK 10
Total Base:100
Chrome Oxide 2
Bentonite 2
Total: 104

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 Cr2O3 LOI
Nepheline Syenite (Theoretical)3018.216.990.030.211.382.944.320.030.21
Silica3030
Gerstley Borate202.960.25.360.73.880.080.80.880.020.080.025.9
Whiting105.614.39
EPK104.573.740.010.020.030.010.040.030.080.041.48
Chrome Oxide22
Bentonite21.190.40.040.020.020.060.080.070.2
Total10456.9311.335.360.789.741.523.815.320.050.260.06212.18
100% no LOI 6212.345.840.8510.611.654.155.80.050.280.062.18

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.23 Na2O
0.06 K2O
0.64 CaO
0.07 MgO
STABILIZERS

R2O3

0.41 Al2O3
0.28 B2O3
GLASS-FORMERS

RO2

3.5 SiO2
OTHER

 

0.01 Fe2O3
0.05 Cr2O3
SILICA:ALUMINA

SiO2:Al2O3

8.53

FLUX RATIO

R2O:RO

0.29 : 0.71

SiO2:Al2O3 Chart

Closest 29 neighbors in Glaze > Green > Chrome.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 8.53

Similar Base Recipes

Δ5 - 6

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Chrome Green 6 0.41 0.28 3.5 0.29 0.06 0.23 0.64 0.07
Odyssey Base w/ 1% Chrome 5-6 0.4 0.29 3.46 0.29 0.06 0.23 0.65 0.07
Celadon 5-6 0.4 0.29 3.46 0.29 0.06 0.23 0.65 0.07

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Gerstley Borate
Whiting Harmful WARNING Causes eye irritation
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Chrome Oxide WARNING May be harmful if inhaled. May cause
irritation to eyes and respiratory tract. Slightly toxic if ingested.
2 0 1 E
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation