Category: Glaze > Raku
Created 2017-03-16 19:41:46 by Jesse VanderBand
Categories: Glaze > Raku
Firing Temperature: Δ06-05
Atmospheres: Raku

Material Amount Batch Subtotal
Colemanite 50
Frit 3134 50
Copper Carbonate 5.6
Tin Oxide 5.1
Total: 110.7

Percentage Analysis

Ingredient Amount SiO2 B2O3 CaO Na2O KNaO CuO SnO2 LOI
Colemanite5025.413.6510.95
Frit 31345023.2511.5410.065.145.14
Copper Carbonate5.63.611.99
Tin Oxide5.15.1
Total110.723.2536.9423.715.145.143.615.112.94
100% no LOI 23.7937.7924.265.265.263.695.22

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.16 Na2O
0.84 CaO
STABILIZERS

R2O3

1.05 B2O3
GLASS-FORMERS

RO2

0.77 SiO2
0.07 SnO2
OTHER

 

0.09 CuO
SILICA:ALUMINA

SiO2:Al2O3

0.00

FLUX RATIO

R2O:RO

0.16 : 0.84

SiO2:Al2O3 Chart

Closest 65 neighbors in Glaze > Raku.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 0

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

No recipes with similar RO/R2O Unity Formulas were found.

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Tin Oxide Harmful WARNING Harmful if swallowed.