Category: Glaze > Red
Created 2017-04-07 16:10:37 by Clara Giorello
Categories: Glaze > Red
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Glossy - Semi
Transparency: Opaque

**David Tsabar recalculation using frit 3134 of a popular Chrome/Tin Red glaze with many names: Scott's Red, June Perry Red, McDonald's Red, Ron Roy Red Burgundy, Purple Red, Raspberry....
Frit 3134 gives pink/purple color and local (Argentina ) frit 804 a nice red.
%analysis frit 804: https://glazy.org/materials/826.
"Maybe" Ferro Frit 3110 can be used for the nice red color.
See pictures with frits 3134 and 804 with different amounts of chrome and tin.
Better results over white body, thick, cone 6 tip touching the shelf. At cone 5 the color is less bright.
**Recálculo hecho por David Tsabar usando frita 3134 de Ferro (174 de Crecer-Argentina) de un esmalte rojo de cromo/estaño muy popular con muchos nombres: Scott's Red, June Perry Red, McDonald's Red, Ron Roy Red Burgundy, Purple Red, Raspberry....
Hice pruebas con Caolín Patagónico y Tinkar Z en vez del caolín. La muestra con Caolín Patagónico parece ofrecer una mejor calidad de esmalte.
También usando la frita 804 de Crecer (Argentina), que parece brindar el mejor rojo. Ver los diferentes resultados con las dos fritas y diferentes cantidades de cromo/estaño.
Mejor resultado sobre pasta blanca, capa más bien gruesa de esmalte y a cono 6. A cono 5 el color es más apagado.

Material Amount Batch Subtotal
Silica 28.5
Frit 3134 25.5
Whiting 21.5
Kaolin (Theoretical) 21.5
Nepheline Syenite (Theoretical) 3
Total Base:100
Tin Oxide 6
Chrome Oxide 0.2
Total: 106.2

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO K2O Na2O KNaO Fe2O3 Cr2O3 SnO2 LOI
Silica28.528.5
Frit 313425.511.865.895.132.622.62
Whiting21.512.069.44
Kaolin (Theoretical)21.510.178.652.69
Nepheline Syenite (Theoretical)31.820.70.020.140.290.430.02
Tin Oxide66
Chrome Oxide0.20.2
Total106.252.359.345.89017.220.142.913.0500.2612.15
100% no LOI 55.669.936.26018.30.153.13.2500.216.38

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.13 Na2O
0.86 CaO
STABILIZERS

R2O3

0.26 Al2O3
0.24 B2O3
GLASS-FORMERS

RO2

2.45 SiO2
0.11 SnO2
SILICA:ALUMINA

SiO2:Al2O3

9.51

FLUX RATIO

R2O:RO

0.14 : 0.86

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Red.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 9.51

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
David Tsabar's Red - Rojo 6 0.26 0.24 2.45 0.11 0.13 0.13 0.86
Wine Red 6 0.24 0.24 2.44 0.1 0.14 0.03 0.11 0.81 0.05
Rodgers Wine Purple 5-6 0.24 0.24 2.44 0.1 0.14 0.03 0.11 0.81 0.05
Ron Roy Red/Burgundy 6 0.24 0.24 2.44 0.1 0.14 0.03 0.11 0.81 0.05

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Whiting Harmful WARNING Causes eye irritation
Kaolin (Theoretical) HarmfulHealth Hazard DANGER SDS for EPK KAOLIN: EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
Tin Oxide Harmful WARNING Harmful if swallowed.
Chrome Oxide WARNING May be harmful if inhaled. May cause
irritation to eyes and respiratory tract. Slightly toxic if ingested.