Category: Glaze > Clear
Created 2017-05-04 19:09:38 by Stacey McDonald
Categories: Glaze > Clear
Firing Temperature: Δ5-6
Atmospheres: Oxidation
Surface Type: Satin - Matte
Transparency: Transparent

Possible colorants: Use any one combination

Nickel 1% produced a pale tan/brown on porcelain
Cobalt Carbonate 1% produced a strong matte blue on porcelain
Rutile 4 – 8 %
Copper Carbonate 1.5 % and Rutile 4% produced a green with brown flecks (un-sieved) on porcelain
Mason Stains – try 3 – 5% for transparent versions. 10% produced strong colors

CMC gum aids in even distribution of the glaze on the work, especially with brushing.

Material Amount Batch Subtotal
Potash Feldspar (Theoretical) 30.3
Nepheline Syenite (Theoretical) 20.2
Whiting 17.17
EPK 14.14
Zinc Oxide 9.09
Silica 5.05
Gerstley Borate 4.04
Total Base:99.99
Bentonite 5
CMC 2
Total: 106.99

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO ZnO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Potash Feldspar (Theoretical)30.319.625.555.135.13
Nepheline Syenite (Theoretical)20.212.264.710.020.140.931.982.910.020.14
Whiting17.179.637.54
EPK14.146.475.280.010.030.050.010.060.040.110.052.09
Zinc Oxide9.099.09
Silica5.055.05
Gerstley Borate4.040.60.041.080.140.780.020.160.180.021.19
Bentonite52.971.010.10.050.050.150.20.180.5
CMC2
Total106.9946.9616.591.080.2810.639.096.172.38.470.040.320.0611.46
100% no LOI 50.2217.731.160.311.379.726.62.469.060.040.340.06

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.09 Na2O
0.16 K2O
0.27 ZnO
0.46 CaO
0.02 MgO
STABILIZERS

R2O3

0.4 Al2O3
0.04 B2O3
GLASS-FORMERS

RO2

1.9 SiO2
SILICA:ALUMINA

SiO2:Al2O3

4.80

FLUX RATIO

R2O:RO

0.25 : 0.75

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Clear.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 4.8

Similar Base Recipes

No recipes with similar base ingredients and amounts were found.

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Heino-Render Satin Matte Clear 5-6 0.4 0.04 1.9 0.25 0.16 0.09 0.46 0.02 0.27
Val Cushing V.C. Med Temp 1 5-6 0.44 1.89 0.28 0.07 0.21 0.47 0.25
Pepin1/VCmatte3 4-6 0.37 1.94 0.24 0.24 0.48 0.28
Pepin2/VCmatte3 4-6 0.37 1.94 0.03 0.24 0.24 0.48 0.28
Emily's Satin Matt 5-6 0.38 1.95 0.21 0.07 0.14 0.51 0.27

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Whiting Harmful WARNING Causes eye irritation
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Zinc Oxide 0 0 0 *
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Gerstley Borate
Bentonite Harmful WARNING Causes eye irritation
Causes skin irritation
May cause respiratory irritation
CMC 0 1 0 *