I've tried the Marilee's lava without adding the stain. It became white and it's quite interesting actually.

Material Amount Batch Subtotal
Custer Feldspar 49.73
Whiting 23.91
EPK 13.18
Silica 13.18
Total Base:100
Titanium Dioxide 11.29
Silicon carbide 0.34
Total: 111.63

Percentage Analysis

Ingredient Amount SiO2 Al2O3 MgO CaO K2O Na2O KNaO P2O5 Fe2O3 TiO2 LOI
Custer Feldspar49.7334.078.450.154.971.496.460.050.15
Whiting23.9113.4110.5
EPK13.186.034.920.010.020.050.010.060.030.10.051.95
Silica13.1813.18
Titanium Dioxide11.2911.29
Silicon carbide0.340.51
Total111.6353.7813.380.0113.595.021.56.520.030.1511.3412.43
100% no LOI 54.4313.540.0113.755.081.526.60.030.1511.48

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.08 Na2O
0.17 K2O
0.76 CaO
STABILIZERS

R2O3

0.41 Al2O3
GLASS-FORMERS

RO2

2.78 SiO2
0.44 TiO2
SILICA:ALUMINA

SiO2:Al2O3

6.76

FLUX RATIO

R2O:RO

0.24 : 0.76

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Specialty.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 6.76

Similar Base Recipes

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
white volcano 6 0.41 2.78 0.44 0.25 0.17 0.08 0.76
Marilee Lava 6 0.41 2.76 0.43 0.25 0.17 0.08 0.76
Marilee's Lava 6 0.41 2.78 0.44 0.25 0.17 0.08 0.76

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Custer Feldspar HarmfulHealth Hazard WARNING May cause damage to lungs through prolonged or repeated inhalation.
Suspected of causing cancer through
prolonged or repeated inhalation.
May cause allergy or asthma symptoms or breathing difficulties if inhaled.
May cause skin or eye irritation.
Whiting Harmful WARNING Causes eye irritation
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Titanium Dioxide Health Hazard WARNING Suspected of causing cancer
Silicon carbide Health Hazard WARNING May cause cancer