Created 2017-05-17 07:51:12 by Jayne Bunting
Categories: Glaze > Blue
Firing Temperature: Δ6
Atmospheres: Oxidation
Surface Type: Glossy
Transparency: Translucent

Used gillespie borate instead of gerstley borate and Cobalt Oxide (div by 1.4) instead of Cobalt Carbonate. Fired to 1222 oC ^6 oxidisation

Results were a little thin & runny next time I will run tests increasing the specific gravity /thickness of application
Increase Rutile to 7.5
Increase Cobalt Oxide to 1-3%

Material Amount Batch Subtotal
Silica 32.8
Nepheline Syenite (Theoretical) 24
Gillespie Borate 16.8
Strontium Carbonate 12
EPK 8
Wollastonite (Theoretical) 6.4
Total Base:100
Copper Carbonate 2.98
Rutile 2.75
Cobalt Oxide 0.11
Total: 105.84

Percentage Analysis

Ingredient Amount SiO2 Al2O3 B2O3 MgO CaO SrO K2O Na2O KNaO P2O5 Fe2O3 TiO2 CoO CuO LOI
Silica32.832.8
Nepheline Syenite (Theoretical)2414.575.590.020.171.12.353.450.020.17
Gillespie Borate16.81.980.294.110.653.860.080.630.635.19
Strontium Carbonate128.423.58
EPK83.662.990.010.010.030.010.040.020.060.031.18
Wollastonite (Theoretical)6.43.313.09
Copper Carbonate2.981.921.06
Rutile2.750.272.48
Cobalt Oxide0.110.10.01
Total105.8456.328.874.110.697.148.51.132.994.120.020.362.510.11.9211.19
100% no LOI 59.59.374.350.737.548.981.23.164.360.020.382.650.112.03

Unity Molecular Formula (UMF)

FLUXES

RO/R2O

0.17 Na2O
0.04 K2O
0.29 SrO
0.44 CaO
0.06 MgO
STABILIZERS

R2O3

0.3 Al2O3
0.21 B2O3
GLASS-FORMERS

RO2

3.27 SiO2
0.11 TiO2
OTHER

 

0.01 Fe2O3
0.08 CuO
SILICA:ALUMINA

SiO2:Al2O3

10.78

FLUX RATIO

R2O:RO

0.21 : 0.79

SiO2:Al2O3 Chart

Closest 100 neighbors in Glaze > Blue.

Click and drag to zoom
Stull Chart
SiO2:Al2O3 Ratio
SiO2:Al2O3 Ratio 10.78

Similar RO/R2O Unity Formulas

R2O3 - STABILIZERS RO2 - GLASS FORMERS RO/R2O - FLUXES
Recipe Name ΔTemp Al2O3 B2O3 SiO2 ZrO2 SnO2 TiO2 KNaO K2O Na2O CaO MgO ZnO BaO PbO Li2O SrO
Kitten's Clear blue/green (Bunty's variation) 6 0.3 0.21 3.27 0.11 0.21 0.04 0.17 0.44 0.06 0.29
Bunty's Variation of Kitten's Clear Blue Rutile 5-6 0.3 0.21 3.27 0.16 0.21 0.04 0.17 0.44 0.06 0.29
Kitten's Clear rutile blue 6 0.31 0.21 3.28 0.16 0.22 0.08 0.14 0.44 0.06 0.29
Kitten's Clear floating blue 6 0.31 0.21 3.28 0.16 0.22 0.08 0.14 0.44 0.06 0.29
Kitten's Clear light blue 6 0.31 0.21 3.28 0.16 0.22 0.08 0.14 0.44 0.06 0.29
Kitten's Clear blue/green 6 0.31 0.21 3.28 0.11 0.22 0.08 0.14 0.44 0.06 0.29
Kitten's Clear green 6 0.31 0.21 3.28 0.16 0.22 0.08 0.14 0.44 0.06 0.29

No reviews yet.

Hazards

09/2016 Note: This is a new feature. If a recipe material is not listed, that material's data has not yet been added. Some materials only have GHS ratings, while others only have HMIS ratings. Warnings differ between systems and countries. Glazy does not take any responsibility for accuracy of linked SDS information. Contact your ceramics supplier for safety information for your specific materials.
Globally Harmonized System (GHS) Hazardous Materials Identification System (HMIS) SDS Link
Material Pictograms Signal Word Hazard Statements Health Flammability Hazard Protection
Silica HarmfulHealth Hazard DANGER From 200-Mesh SDS:
May cause cancer by inhalation.
Causes damage to lungs through prolonged or repeated exposure by inhalation.
* 0 0 E
Strontium Carbonate Harmful WARNING Product dust may be irritating to eyes,skin and respiratory system.  1 0 0 E
EPK HarmfulHealth Hazard DANGER EPK Kaolin is a naturally occurring mineral, which may contain amounts of crystalline silica
typically 0.1-1.0%, may cause damage to respiratory system through prolonged or repeated
exposure.
1 0 0 E
Wollastonite (Theoretical) Health Hazard DANGER Vansil W-30 Wollastonite SDS:
May cause cancer if inhaled.
Causes damage to organs through prolonged or repeated exposure if inhaled. (respiratory tract)
Copper Carbonate Harmful WARNING Harmful if swallowed.
Causes skin irritation.
Causes serious eye irritation.
Rutile 1 0 0
Cobalt Oxide HarmfulHealth Hazard WARNING Suspected of causing cancer
Harmful if swallowed
May cause allergy or breathing difficulties if inhaled
May cause an allergic skin reaction
2 0 0 *